Difference between revisions of "MainPage:Nuclear:NPS:PWO:CrystalLOG:SICCAJ35"

From cua_phy
Jump to navigation Jump to search
Line 27: Line 27:
 
|-
 
|-
 
| 05/20/2016 || Transverse Transmittance Scan || Wavelengths: 360nm, 420nm, 620nm. Sampling period: 0.6s, moving motor at 2mm/s.
 
| 05/20/2016 || Transverse Transmittance Scan || Wavelengths: 360nm, 420nm, 620nm. Sampling period: 0.6s, moving motor at 2mm/s.
 +
|-
 +
| 07/07/2016 || Longitudinal Transmittance Scan || Wavelengths: 200-800 nm. Sampling period: 0.6s, moving motor at 2mm/s.
 
|}
 
|}
  

Revision as of 11:17, 19 July 2016

⇐ Back to Crystal LOG
⇐ Back to Neutral Particle Spectrometer
⇐ Back to the Main_Page

Time LOG

SICCA J35
Date Description Comments
03/17/2016 Pictures Documentation of crystal's conditions as it arrived at CUA.
03/18/2016 Thermal annealing Ramp up at 18oC/hour up to 200oC. Stays for 10 hours and ramp down at 18oC/hour.
04/24/2016 Light Yield Run 3196: crystal wrapped with ~5 layers of teflon tape and 2 layers of black tape. Steps of 20min, 1cm. T=18oC. LY = 16.1161 ± 0.566 pe/MeV.
05/17/2016 Transverse Transmittance At the center of the crystal, every nm from 200nm until 800nm. Sample: 1351
05/20/2016 Transverse Transmittance Scan Wavelengths: 360nm, 420nm, 620nm. Sampling period: 0.6s, moving motor at 2mm/s.
07/07/2016 Longitudinal Transmittance Scan Wavelengths: 200-800 nm. Sampling period: 0.6s, moving motor at 2mm/s.